Tantalum hydride, R0 = 15.100 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.197    2.880    6.320     229.522     1.534   23.1672      4.147         1
  1.201    4.230    8.250     438.662     1.708   25.7966      8.946         1
  1.202    0.410    2.220      11.432     1.020   15.4051      0.084         1
  1.202    0.780    3.170      31.056     1.103   16.6591      0.304         1
  1.204    2.330    5.720     167.128     1.401   21.1589      2.714         1
  1.208    0.490    2.430      14.884     1.037   15.6572      0.120         1
  1.211    1.290    4.120      66.276     1.202   18.1542      0.832         1
  1.212    2.650    5.990     197.784     1.480   22.3459      3.511         1
  1.213    0.880    3.330      36.484     1.121   16.9218      0.387         1
  1.226    1.740    4.800     102.897     1.280   19.3255      1.514         1
  1.380    0.990    2.860      30.976     1.108   16.7318      0.490         1
  1.383    2.790    6.060     184.629     1.340   20.2371      3.892         1
  1.383    3.090    6.100     205.831     1.466   22.1302      4.774         1
  1.384    1.870    4.520      92.216     1.232   18.6088      1.748         1

References:
1. R. F. Trunin, M. V. Zhernokletov, N. F. Kuznetsov, Yu. N. Sutulov, Shock
   compressibility of hydrides of metalls, Fiz. Zemli. 11, 65-70 (1987) [in
   Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g