Titanum hydride, R0 =  3.780 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.041    0.760    5.790      15.974     1.105    4.1785      0.289         1
  1.041    1.030    6.320      23.630     1.147    4.3368      0.530         1
  1.044    0.700    5.690      14.419     1.092    4.1278      0.245         1
  1.044    2.270    7.780      63.931     1.352    5.1114      2.576         1
  1.044    3.070    8.900      98.909     1.462    5.5262      4.712         1
  1.044    3.400    9.400     115.695     1.500    5.6713      5.780         1
  1.044    3.720    9.950     133.991     1.530    5.7815      6.919         1
  1.044    5.630   12.330     251.293     1.762    6.6619     15.848         1
  1.047    1.340    6.720      32.507     1.193    4.5091      0.898         1
  1.047    2.700    8.360      81.485     1.411    5.3321      3.645         1
  1.053    1.840    7.370      48.683     1.266    4.7845      1.693         1
  1.053    2.510    8.020      72.268     1.382    5.2254      3.150         1
  1.053    3.060    8.770      96.342     1.459    5.5139      4.682         1

References:
1. R. F. Trunin, M. V. Zhernokletov, N. F. Kuznetsov, Yu. N. Sutulov, Shock
   compressibility of hydrides of metalls, Fiz. Zemli. 11, 65-70 (1987) [in
   Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g