Gadolinium, R0 =  7.930 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.600    2.830      13.465     1.269   10.0636      0.180         1
  1.000    1.280    3.510      35.628     1.574   12.4817      0.819         1
  1.000    2.330    4.790      88.504     1.947   15.4409      2.714         1
  1.000    3.480    6.260     172.754     2.252   17.8568      6.055         1
  1.000    5.000    8.290     328.699     2.520   19.9817     12.500         1
  1.000    0.360    2.670       7.622     1.156    9.1658      0.065         2
  1.000    1.420    3.600      40.538     1.651   13.0954      1.008         2
  1.000    2.760    5.260     115.125     2.104   16.6847      3.809         2
  1.005    0.670    2.860      15.119     1.299   10.3038      0.224         2
  1.005    1.050    3.150      26.096     1.492   11.8350      0.551         2
  1.005    1.940    4.310      65.972     1.809   14.3485      1.882         2
  1.009    0.000    2.212       0.000     0.991    7.8610      0.000         3
  1.009    0.324    2.494       6.352     1.139    9.0347      0.052         3
  1.009    0.442    2.610       9.069     1.193    9.4637      0.098         3
  1.009    0.673    2.802      14.824     1.305   10.3459      0.226         3
  1.009    0.691    2.824      15.340     1.312   10.4076      0.239         3
  1.009    0.865    2.993      20.352     1.394   11.0564      0.374         3
  1.009    1.080    3.219      27.329     1.492   11.8301      0.583         3
  1.009    1.082    3.205      27.261     1.497   11.8674      0.585         3
  1.009    1.135    3.221      28.739     1.531   12.1382      0.644         3
  1.009    1.219    3.353      32.130     1.558   12.3514      0.743         3
  1.009    1.268    3.364      33.532     1.591   12.6166      0.804         3
  1.009    1.347    3.481      36.860     1.617   12.8229      0.907         3
  1.009    1.582    3.812      47.407     1.695   13.4377      1.251         3
  1.009    1.916    4.276      64.404     1.796   14.2431      1.836         3
  1.009    2.146    4.613      77.820     1.854   14.6991      2.303         3
  1.009    2.179    4.567      78.229     1.896   15.0340      2.374         3
  1.009    2.206    4.574      79.320     1.915   15.1842      2.433         3
  1.009    2.373    4.822      89.950     1.952   15.4780      2.816         3
  1.009    2.401    4.885      92.201     1.949   15.4593      2.882         3
  1.009    2.639    5.161     107.066     2.029   16.0867      3.482         3
  1.009    2.718    5.253     112.237     2.054   16.2895      3.694         3
  1.009    2.759    5.395     117.010     2.029   16.0888      3.806         3
  1.009    3.073    5.618     135.713     2.188   17.3529      4.722         3
  1.009    3.098    5.806     141.396     2.125   16.8541      4.799         3
  1.009    3.104    5.726     139.718     2.165   17.1671      4.817         3
  1.009    3.142    5.735     141.650     2.192   17.3864      4.936         3
  1.009    3.199    5.739     144.321     2.240   17.7615      5.117         3
  1.000    7.020   10.730     597.324     2.892   22.9350     24.640         4

References:
1. L. V. Al'tshuler, A. A. Bakanova, I. P. Dudoladov, Effect of electrons
   structure on the shock compressibility of metals at high pressure, Zh. Eksp.
   Teor. Fiz. 53, 1967-1976 (1967) [in Russian] (Sov. Phys. - JETP 26(6),
   1115-1120 (1968))
2. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977)
3. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)
4. L. V. Al'tshuler, A. A. Bakanova, I. P. Dudoladov, E. A. Dynin, R. F. Trunin,
   B. S. Chekin, Shock adiabats for metals. New data, statistical analysis and
   general regularities, Zh. Prikl. Mekh. Tekhn. Fiz. 2, 3-34 (1981) [in Russian]
   (J. Appl. Mech. Techn. Phys. 22, 145 (1981))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g