Epoxy compound EK-34, R0 =  1.170 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    2.110    5.830      14.393     1.567    1.8336      2.226         1
  1.000    2.820    6.900      22.766     1.691    1.9787      3.976         1
  1.000    3.730    7.840      34.215     1.908    2.2318      6.956         1
  1.000    5.010    9.360      54.866     2.152    2.5175     12.550         1

References:
1. R. F. Trunin, L.F.Gudarenko, M. V. Zhernokletov, G. V. Simakov, Experimental
   data on shock compressibility and adiabatic expansion of condensed substances,
   RFNC, Sarov (2001) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g