Holmium, R0 =  8.734 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.000    2.386       0.000     1.000    8.7340      0.000         1
  1.000    0.423    2.680       9.901     1.187   10.3709      0.089         1
  1.000    0.643    2.878      16.163     1.288   11.2467      0.207         1
  1.000    0.659    2.914      16.772     1.292   11.2864      0.217         1
  1.000    0.828    3.060      22.129     1.371   11.9740      0.343         1
  1.000    1.172    3.393      34.732     1.528   13.3428      0.687         1
  1.000    1.216    3.430      36.429     1.549   13.5310      0.739         1
  1.000    1.293    3.534      39.910     1.577   13.7733      0.836         1
  1.000    1.365    3.554      42.371     1.624   14.1803      0.932         1
  1.000    1.389    3.632      44.062     1.619   14.1426      0.965         1
  1.000    1.520    3.819      50.700     1.661   14.5085      1.155         1
  1.000    1.529    3.809      50.867     1.671   14.5911      1.169         1
  1.000    1.674    3.877      56.685     1.760   15.3707      1.401         1
  1.000    1.931    4.299      72.504     1.815   15.8562      1.864         1
  1.000    1.991    4.236      73.662     1.887   16.4798      1.982         1
  1.000    2.085    4.517      82.256     1.857   16.2218      2.174         1
  1.000    2.121    4.452      82.473     1.910   16.6812      2.249         1
  1.000    2.675    5.178     120.976     2.069   18.0682      3.578         1
  1.000    2.975    5.585     145.119     2.140   18.6894      4.425         1
  1.000    3.025    5.560     146.897     2.193   19.1562      4.575         1
  1.000    0.570    2.840      14.139     1.251   10.9271      0.162         2
  1.000    1.240    3.440      37.256     1.564   13.6568      0.769         2
  1.000    2.250    4.600      90.397     1.957   17.0963      2.531         2
  1.000    3.300    6.100     175.816     2.179   19.0276      5.445         2
  1.000    4.820    8.340     351.096     2.369   20.6936     11.616         2

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)
2. L. V. Al'tshuler, A. A. Bakanova, I. P. Dudoladov, E. A. Dynin, R. F. Trunin,
   B. S. Chekin, Shock adiabats for metals. New data, statistical analysis and
   general regularities, Zh. Prikl. Mekh. Tekhn. Fiz. 2, 3-34 (1981) [in Russian]
   (J. Appl. Mech. Techn. Phys. 22, 145 (1981))

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g