RDX -20 wt% aluminum - 6 wt% wax, R0 =  1.812 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.394    3.377       2.411     1.132    2.0513      0.078    1    1
  1.000    0.468    3.564       3.022     1.151    2.0859      0.110    1    1
  1.000    0.565    3.627       3.713     1.185    2.1464      0.160    1    1
  1.000    0.997    4.016       7.255     1.330    2.4104      0.497    1    1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Remarks:
1. 30-micron aluminum

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g