TATB -5 wt% B square wax - 5 wt% Elvax, R0 =  1.740 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.012    4.489       7.905     1.291    2.2464      0.512         1
  1.000    1.543    5.444      14.616     1.396    2.4282      1.190         1
  1.000    1.672    6.302      18.334     1.361    2.3684      1.398         1
  1.000    1.703    5.901      17.486     1.406    2.4459      1.450         1
  1.000    1.834    6.224      19.862     1.418    2.4669      1.682         1
  1.000    1.904    6.180      20.474     1.445    2.5148      1.813         1
  1.000    1.909    6.441      21.395     1.421    2.4729      1.822         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g