TATB - 10 wt% Kel F 800, Pantex standard TATB, R0 =  1.912 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.942    4.363       7.858     1.275    2.4385      0.444         1
  1.000    1.114    4.596       9.789     1.320    2.5237      0.621         1
  1.000    1.125    4.590       9.873     1.325    2.5328      0.633         1
  1.000    1.218    4.931      11.483     1.328    2.5392      0.742         1
  1.000    1.256    4.755      11.419     1.359    2.5983      0.789         1
  1.000    1.302    5.375      13.381     1.320    2.5232      0.848         1
  1.000    1.369    5.543      14.509     1.328    2.5391      0.937         1
  1.000    1.388    5.302      14.071     1.355    2.5900      0.963         1
  1.000    1.390    5.340      14.192     1.352    2.5848      0.966         1
  1.000    1.455    5.664      15.757     1.346    2.5730      1.059         1
  1.000    1.458    5.473      15.257     1.363    2.6063      1.063         1
  1.000    1.470    5.413      15.214     1.373    2.6248      1.080         1
  1.000    1.532    5.448      15.958     1.391    2.6600      1.174         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g