TATB - 15 wt% Kel F 800, 1968 TATB, R0 =  1.930 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.380    5.371      14.305     1.346    2.5974      0.952         1
  1.000    1.476    5.477      15.602     1.369    2.6420      1.089         1
  1.000    1.575    5.638      17.138     1.388    2.6782      1.240         1
  1.000    1.684    5.749      18.685     1.414    2.7295      1.418         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g