TATB - 2.5 wt% Kel F 800, - 2.5 wt% Kel F 827, 1968 TATB, R0 =  1.883 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.030    4.524       8.774     1.295    2.4381      0.530         1
  1.000    1.339    5.434      13.701     1.327    2.4987      0.896         1
  1.000    1.462    5.683      15.645     1.346    2.5352      1.069         1
  1.000    1.545    6.014      17.496     1.346    2.5340      1.194         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g