TATB - 7.5 wt% Kel F 800, - 7.5 wt% Kel F 827, 1968 TATB, R0 =  1.912 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.341    5.141      13.182     1.353    2.5867      0.899         1
  1.000    1.381    5.462      14.422     1.338    2.5590      0.954         1
  1.000    1.707    5.722      18.675     1.425    2.7249      1.457         1

References:
1. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g