Lithium iodide, R0 =  4.013 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.270    4.010      20.437     1.464    5.8730      0.806         1
  1.000    1.580    4.240      26.884     1.594    6.3967      1.248         1
  1.000    1.780    4.470      31.930     1.662    6.6684      1.584         1
  1.062    0.690    3.280       8.553     1.193    4.7858      0.238         1
  1.062    1.270    3.780      18.142     1.418    5.6911      0.806         1
  1.062    1.270    3.900      18.717     1.396    5.6038      0.806         1
  1.062    1.610    4.230      25.736     1.520    6.1012      1.296         1
  1.151    0.890    3.720      11.542     1.142    4.5823      0.396         1
  1.211    1.880    4.610      28.713     1.394    5.5945      1.767         1

References:
1. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977), 444-449

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g