Rubidium iodide, R0 =  3.470 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    1.110    3.010      11.594     1.584    5.4972      0.616    1    1
  1.000    1.370    3.440      16.354     1.662    5.7666      0.938    1    1
  1.000    1.730    3.950      23.712     1.779    6.1741      1.496    1    1
  1.000    1.910    4.240      28.102     1.820    6.3145      1.824    1    1

References:
1. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977), 477-482

Remarks:
1. Pressed

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g