Lead epon, R0 =  4.850 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.930    3.270      14.749     1.397    6.7776      0.432         1
  1.000    0.990    3.280      15.749     1.432    6.9467      0.490         1
  1.000    1.220    3.660      21.656     1.500    7.2750      0.744         1
  1.000    1.380    3.870      25.902     1.554    7.5380      0.952         1
  1.000    1.640    4.200      33.407     1.641    7.9570      1.345         1

References:
1. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977), 640-649

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g