Epoxy armstrong C-7 - Activator R, R0 =  1.205 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.600    3.690       2.668     1.194    1.4390      0.180         1
  1.000    0.790    4.010       3.817     1.245    1.5006      0.312         1
  1.000    1.180    4.640       6.598     1.341    1.6160      0.696         1
  1.000    1.530    5.240       9.661     1.412    1.7019      1.170         1
  1.000    1.660    5.380      10.762     1.446    1.7427      1.378         1
  1.000    1.940    5.700      13.325     1.516    1.8267      1.882         1
  1.000    2.350    6.500      18.406     1.566    1.8873      2.761         1
  1.000    2.420    6.460      18.838     1.599    1.9268      2.928         1
  1.000    2.450    6.460      19.072     1.611    1.9412      3.001         1

References:
1. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977), 741-746

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g