Glass cloth 181 laninate with aluminium phosphate resin, R0 =  2.000 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.870    3.180       5.533     1.377    2.7532      0.378         1
  1.000    1.150    3.480       8.004     1.494    2.9871      0.661         1
  1.000    2.200    4.840      21.296     1.833    3.6667      2.420         1
  1.000    2.330    5.100      23.766     1.841    3.6823      2.714         1
  1.070    0.850    3.100       4.925     1.288    2.5751      0.361         1
  1.070    0.860    2.900       4.661     1.328    2.6569      0.370         1
  1.070    1.580    3.660      10.808     1.644    3.2887      1.248         1
  1.070    1.710    3.840      12.273     1.685    3.3695      1.462         1
  1.070    1.780    4.020      13.374     1.677    3.3542      1.584         1
  1.070    2.180    4.490      18.294     1.816    3.6328      2.376         1
  1.070    2.340    4.790      20.949     1.827    3.6541      2.738         1
  1.070    2.470    4.850      22.390     1.904    3.8087      3.050         1
  1.169    0.730    2.490       3.110     1.210    2.4207      0.266         1
  1.169    0.890    2.530       3.853     1.320    2.6395      0.396         1
  1.169    2.450    4.600      19.283     1.830    3.6607      3.001         1
  1.169    2.480    4.640      19.689     1.838    3.6755      3.075         1

References:
1. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977), 741-746

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g