Bismut, liquid, To=673 K, R0 =  9.890 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.420    2.650      11.008     1.188   11.7527      0.088         1
  1.000    0.680    2.970      19.974     1.297   12.8268      0.231         1
  1.000    0.970    3.330      31.946     1.411   13.9550      0.470         1
  1.000    1.460    3.990      57.613     1.577   15.5973      1.066         1
  1.000    1.920    4.690      89.058     1.693   16.7452      1.843         1
  1.000    2.600    5.610     144.256     1.864   18.4329      3.380         1

References:
1. R. F. Trunin, M. V. Zhernokletov, N. F. Kuznetsov, V. V. Shutov, Dynamical
   compressibility of melted and cooled metals, Teplofiz. Vys. Temp. 33(2),
   222-226 (1995) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g