Bismut, cooled, To=78 K, R0 =  9.846 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.460    2.190       9.919     1.266   12.4640      0.106         1
  1.000    0.710    2.630      18.386     1.370   13.4870      0.252         1
  1.000    1.000    3.120      30.720     1.472   14.4903      0.500         1
  1.000    1.450    3.930      56.108     1.585   15.6027      1.051         1
  1.000    1.730    4.320      73.585     1.668   16.4227      1.496         1
  1.000    1.930    4.620      87.793     1.717   16.9102      1.862         1
  1.000    2.580    5.670     144.033     1.835   18.0669      3.328         1
  1.000    2.890    6.140     174.713     1.889   18.6014      4.176         1

References:
1. R. F. Trunin, M. V. Zhernokletov, N. F. Kuznetsov, V. V. Shutov, Dynamical
   compressibility of melted and cooled metals, Teplofiz. Vys. Temp. 33(2),
   222-226 (1995) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g