Copper, heated, To=673 K, R0 =  8.750 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.580    4.780      24.259     1.138    9.9583      0.168         1
  1.000    0.870    4.930      37.530     1.214   10.6250      0.378         1
  1.000    1.320    5.730      66.182     1.299   11.3690      0.871         1
  1.000    1.780    6.430     100.147     1.383   12.0995      1.584         1
  1.000    2.430    7.510     159.681     1.478   12.9355      2.952         1
  1.000    2.730    8.080     193.011     1.510   13.2150      3.726         1

References:
1. R. F. Trunin, M. V. Zhernokletov, N. F. Kuznetsov, V. V. Shutov, Dynamical
   compressibility of melted and cooled metals, Teplofiz. Vys. Temp. 33(2),
   222-226 (1995) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g