Cadmium, liquid, To=673 K, R0 =  7.930 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    0.700    3.480      19.318     1.252    9.9268      0.245         1
  1.000    0.960    3.880      29.538     1.329   10.5371      0.461         1
  1.000    1.490    4.700      55.534     1.464   11.6109      1.110         1
  1.000    1.960    5.530      85.952     1.549   12.2837      1.921         1
  1.000    2.650    6.630     139.326     1.666   13.2100      3.511         1
  1.000    2.960    7.180     168.535     1.701   13.4923      4.381         1

References:
1. R. F. Trunin, M. V. Zhernokletov, N. F. Kuznetsov, V. V. Shutov, Dynamical
   compressibility of melted and cooled metals, Teplofiz. Vys. Temp. 33(2),
   222-226 (1995) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g