Stishovite, R0 =  4.310 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.000    2.060   11.630     103.258     1.215    5.2378      2.122         1
  1.000    3.050   12.760     167.737     1.314    5.6638      4.651         1
  1.000    3.380   13.300     193.752     1.341    5.7785      5.712         1
  1.000    3.920   13.890     234.674     1.393    6.0046      7.683         1

References:
1. S. N. Luo, J. L. Mosenfelder, P. D. Asimov, T. J. Ahrens, Direct shock wave
   loading of stishovite to 235 GPa: Implications for perovskite stability
   relative to an oxide assemblage at lower mantle conditions, Gephys. Res.
   Lett., 29(14) (2002).

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g