Scanduim, R0 =  3.195 g/cc

    m        U        D           P        R/R0      R         E-E0    Rem  Ref
  1.034    0.690    5.630      12.004     1.102    3.5216      0.238         1
  1.034    1.560    6.090      29.356     1.300    4.1541      1.217         1
  1.034    2.930    7.310      66.183     1.614    5.1571      4.292         1
  1.034    4.160    8.420     108.234     1.912    6.1075      8.653         1
  1.034    6.040   10.940     204.180     2.159    6.8989     18.241         1
  1.000    0.530    4.950       8.382     1.120    3.5781      0.140         2
  1.000    0.580    5.070       9.395     1.129    3.6077      0.168         2
  1.000    1.290    5.660      23.328     1.295    4.1381      0.832         2
  1.000    1.680    5.960      31.991     1.393    4.4491      1.411         2
  1.000    2.500    6.710      53.596     1.594    5.0923      3.125         2
  1.000    3.360    7.370      79.119     1.838    5.8721      5.645         2
  1.000    0.750    5.270      12.628     1.166    3.7251      0.281         3
  1.000    0.950    5.320      16.148     1.217    3.8896      0.451         3
  1.000    1.400    5.670      25.362     1.328    4.2425      0.980         3
  1.000    1.930    6.020      37.122     1.472    4.7027      1.862         3
  1.000    2.580    6.690      55.146     1.628    5.2006      3.328         3
  1.000    3.000    7.040      67.478     1.743    5.5675      4.500         3
  1.000    3.750    7.830      93.813     1.919    6.1316      7.031         3
  1.000    0.000    4.296       0.000     1.000    3.1950      0.000         4
  1.000    0.755    5.274      12.722     1.167    3.7288      0.285         4
  1.000    0.948    5.317      16.105     1.217    3.8883      0.449         4
  1.000    1.405    5.670      25.453     1.329    4.2475      0.987         4
  1.000    1.932    6.017      37.141     1.473    4.7061      1.866         4
  1.000    2.578    6.693      55.128     1.626    5.1966      3.323         4
  1.000    3.003    7.038      67.527     1.744    5.5728      4.509         4
  1.000    3.752    7.833      93.899     1.919    6.1324      7.039         4

References:
1. L. V. Al'tshuler, A. A. Bakanova, I. P. Dudoladov, Effect of electrons
   structure on the shock compressibility of metals at high pressure, Zh. Eksp.
   Teor. Fiz. 53, 1967-1976 (1967) [in Russian] (Sov. Phys. - JETP 26(6),
   1115-1120 (1968))
2. W. H. Gust, E. B. Royce, New Electronic Interactions in Rare-Earth Metals at
   High Pressure. Phys. Rev. Ser. B, 8, 3595-3609 (1973)
3. W. J. Carter, J. N. Fritz, S. P. Marsh, R. G. McQueen, Hugoniot equation of
   state of the lanthanides, J. Phys. Chem. Solids, 36, 741-752 (1975)
4. S. P. Marsh (Ed.), LASL Shock Hugoniot Data, (Univ. California Press,
   Berkeley, 1980)

Denotions:
R0   - normal density of substance, g/cc
R00  - initial density of sample, g/cc
P0   - initial gas pressure (for gaseous substances only), GPa
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g