Epoxy, R0 =  1.200 g/cc

    m        U0       P0       U        P     Rem  Ref
  1.000    0.767    3.599    1.535    0.004    1    1
  1.000    0.793    3.540    1.586    0.004    1    1
  1.000    1.570   10.117    3.173    0.014    1    1
  1.000    2.261   17.419    4.658    0.030    1    1
  1.005    0.760    3.689    1.520    0.004    2    1
  1.005    1.609   10.221    3.251    0.015    2    1
  1.005    1.998   14.540    4.069    0.023    2    1
  1.005    2.437   18.841    5.026    0.035    2    1
  1.000    3.200   29.031    6.275    0.053         2
  1.000    3.310   30.028    6.275    0.053         2
  1.000    3.843   38.046    8.365    0.090         2

References:
1. D. E. Munson, R. P. May, Dynamically determined high-pressure
   compressibilities of three epoxy systems, J. Appl. Phys. 43(3), 962-971 (1972)
2. A. V. Bushman, V. P. Efremov, V. E. Fortov, G. I. Kanel', I. V. Lomonosov, V.
   Ya. Ternovoi, A. V. Utkin, Equation of state of composites under high energy
   densities, in: Shock Compression of Condensed Matter - 1991 (North Holland,
   Amsterdam, 1992), 79-82

Remarks:
1. Epon 828-Z
2. Epon 828-MPDA

Denotions:
R0 - normal density of substance, g/cc
m  - porosity of sample
U0 - particle velocity on shock Hugoniot, km/s
P0 - pressure on shock Hugoniot, GPa
U  - particle velocity, km/s
P  - pressure, GPa