Magnesium, R0 =  1.740 g/cc

    m        U0       P0       U        P     Rem  Ref
  1.000    2.460   32.000    4.850    0.031         1
  1.000    3.270   49.000    6.770    0.060         1
  1.000    3.900   60.000    8.200    0.081         1
  1.000    3.990   66.000    8.360    0.090         1
  1.000    4.400   76.000    9.450    0.115         1
  1.000    4.780   87.000   10.280    0.137         1

References:
1. A. A. Bakanova, I. P. Dudoladov, M. V. Zhernokletov, V. N. Zubarev, G. V.
   Simakov, On evaporation of shock-compressed metals under expansion, Zh. Prikl.
   Mekh. Tekhn. Fiz., 2, 76-81 (1983) [in Russian] (J. Appl. Mech. Techn. Phys.
   24, 204 (1983))

Denotions:
R0 - normal density of substance, g/cc
m  - porosity of sample
U0 - particle velocity on shock Hugoniot, km/s
P0 - pressure on shock Hugoniot, GPa
U  - particle velocity, km/s
P  - pressure, GPa