Polytetrafluoroethylene (Teflon), R0 =  2.204 g/cc

    m        U        D        Cs          P        R/R0      R          E-E0   Rem  Ref
  1.006    1.210    3.988    5.300      10.568     1.426    3.1439      0.732         1
  1.006    1.520    4.548    5.800      15.139     1.492    3.2893      1.155         1
  1.006    1.450    4.458    5.680      14.156     1.473    3.2457      1.051         2
  1.006    1.860    5.158    6.590      21.011     1.554    3.4251      1.730         2

References:
1. N. T. Kalashnikov, L. V. Kuleshova, M. N. Pavlovskii, Shock compression of
   polytetrafluoroethylene up to pressures 1.7 Mbar, Zh. Prikl. Mekh. Tekhn. Fiz.
   4, 187-191 (1972) [in Russian]
2. M. N. Pavlovskii, Measurements of sound velocity in quartzite, dolomite,
   anhydrite, sodiumn cloride, paraffin, plexiglas, polyethilene, and
   fluoroplast-4 under shock compression, Zh. Prikl. Mekh. Tekhn. Fiz. 5, 136-139
   (1976) [in Russian]

Denotions:
R0   - normal density of substance, g/cc
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
Cs   - sound velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g