Iron, R0 =  7.873 g/cc

    m        U        D        Cs          P        R/R0      R          E-E0   Rem  Ref
  1.000    0.961    5.485    6.120      41.499     1.212    9.5454      0.462         1
  1.000    1.180    5.834    6.700      54.199     1.254    9.8692      0.696         1
  1.000    2.135    7.335    7.850     123.293     1.411   11.1055      2.279         1
  1.000    2.630    8.114    8.490     168.009     1.480   11.6487      3.458         1
  1.000    3.696    9.791    9.530     284.905     1.606   12.6472      6.830         1
  1.000    4.184   10.558    9.980     347.787     1.656   13.0410      8.753         1
  1.000    3.479    9.470    9.510     259.385     1.581   12.4449      6.052         2
  1.000    3.521    9.534    9.490     264.291     1.586   12.4832      6.199         2
  1.000    4.060   10.405   10.030     332.589     1.640   12.9107      8.242         2

References:
1. L. V. Al'tshuler, S. B. Kormer, M. I. Brazhnik, L. A. Vladimirov, M. P.
   Speranskaya, A. I. Funtikov, The isentropic compressibility of aluminum,
   copper, lead at high pressures, Zh. Eksp. Teor. Fiz. 38(4), 1061-1073 (1960)
   [in Russian] (Sov. Phys. - JETP 11(4), 766-775 (1960))
2. J. M. Brown, R. G. McQueen, Phase transitions, Gruneisen parameter, and
   elascticity for shocked iron between 77 GPa and 400 GPa, J. Geophys. Res. Ser.
   B. 91(7), 7485-7494 (1986)

Denotions:
R0   - normal density of substance, g/cc
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
Cs   - sound velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g