Copper, R0 =  8.930 g/cc

    m        U        D        Cs          P        R/R0      R          E-E0   Rem  Ref
  1.000    1.066    5.505    5.950      52.404     1.240   11.0745      0.568         1
  1.000    1.317    5.884    6.320      69.201     1.288   11.5052      0.867         1
  1.000    1.781    6.577    6.710     104.603     1.371   12.2462      1.586         1
  1.000    2.132    7.101    7.130     135.194     1.429   12.7615      2.273         1
  1.000    2.484    7.628    7.780     169.205     1.483   13.2422      3.085         1
  1.000    3.697    9.441    8.930     311.687     1.644   14.6776      6.834         1
  1.000    4.182   10.165    9.480     379.615     1.699   15.1719      8.745         1
  1.000    3.740    9.520    9.050     317.951     1.647   14.7082      6.994         2
  1.000    3.880    9.720    9.170     336.783     1.664   14.8629      7.527         2
  1.000    4.050    9.970    9.300     360.580     1.684   15.0392      8.201         2

References:
1. L. V. Al'tshuler, S. B. Kormer, M. I. Brazhnik, L. A. Vladimirov, M. P.
   Speranskaya, A. I. Funtikov, The isentropic compressibility of aluminum,
   copper, lead at high pressures, Zh. Eksp. Teor. Fiz. 38(4), 1061-1073 (1960)
   [in Russian] (Sov. Phys. - JETP 11(4), 766-775 (1960))
2. D. Hayes, R. S. Hixson, R. G. McQueen, High pressure elastic properties,
   solid-liquid phase boundary and liquid equation of state from release wave
   measurements in shock-loaded copper, in: Shock Compression of Condensed Matter
   - 1999 (AIP Conference Proceedings 505, Eds M. D. Furnish, L. C. Chhabildas,
   R. S. Hixson) (Melville, New York, 2000), 483-488

Denotions:
R0   - normal density of substance, g/cc
m    - porosity of sample
U    - particle velocity, km/s
D    - shock wave velocity, km/s
Cs   - sound velocity, km/s
P    - pressure behind shock front, GPa
R/R0 - compression ratio behind shock front
R    - density behind shock front, g/cc
E-E0 - specific energy behind shock front, kJ/g