Polymethylmethacrylate (Plexiglas), R0 =  1.186 g/cc

Target: PMMA (polymethyl methacrylate)
  Sample density R0 = 1.186 g/cc, bulk sound velocity C0 = 2.65 km/s, longitudial sound velocity Cl = 2.72 km/s
  Sample thickness 8.32 mm 
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.010    200.000
      0.020    370.000
      0.022    377.000
      0.025    382.000
      0.030    387.000
      0.040    390.000
      0.050    391.000
      0.060    390.000
      0.070    388.000
      0.080    385.000
      0.089    380.811
      0.100    374.000
      0.150    348.000
      0.200    322.000
      0.250    296.000
      0.300    269.000
      0.330    257.000
      0.340    255.000
      0.350    254.000
      0.360    257.000
      0.370    263.000
      0.380    270.000
      0.390    276.000
      0.400    280.000
      0.410    282.000
      0.420    283.000
      0.430    278.000
      0.440    277.000
      0.450    276.000
      0.470    270.000
      0.500    268.000
      0.510    265.000
      0.520    263.000
      0.530    260.000
      0.540    259.000
      0.550    258.000
      0.560    253.000
      0.580    250.000
      0.590    244.000
      0.620    242.000
      0.640    237.000
      0.660    235.000
      0.680    233.000
      0.700    231.000
      0.710    232.000
      0.720    240.000
      0.725    245.000
      0.730    247.000
      0.740    249.000
      0.750    250.000
      0.770    249.500
      0.780    249.000
      0.800    248.000
      0.820    247.500
      0.850    243.000
      0.870    239.000
      0.900    236.000
      0.910    233.000
      0.930    233.000
      0.950    229.000
      0.980    223.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)