Polymethylmethacrylate (Plexiglas), R0 =  1.186 g/cc

Target: PMMA (polymethyl methacrylate)
  Sample density R0 = 1.186 g/cc, bulk sound velocity C0 = 2.65 km/s, longitudial sound velocity Cl = 2.72 km/s
  Sample thickness 8.2 mm 
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 1900 +/- 50 m/s
Experiment type: Laser interferometer (VISAR) (hexane window)

     t, mks     V, m/s

      0.000      0.000
      0.020    399.000
      0.020   1210.000
      0.020   1510.000
      0.025   1532.000
      0.030   1540.000
      0.040   1547.000
      0.050   1549.000
      0.060   1548.500
      0.070   1544.000
      0.080   1540.000
      0.100   1530.000
      0.150   1498.000
      0.200   1458.000
      0.250   1424.000
      0.300   1388.000
      0.350   1362.000
      0.400   1337.000
      0.450   1319.000
      0.500   1305.000
      0.550   1297.000
      0.600   1292.000
      0.650   1287.000
      0.700   1281.000
      0.750   1276.000
      0.800   1269.000
      0.850   1258.000
      1.000   1227.000
      1.100   1205.000
      1.200   1185.000
      1.300   1169.000
      1.400   1154.000
      1.480   1144.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)