Polymethylmethacrylate (Plexiglas), R0 =  1.186 g/cc

Target: PMMA (polymethyl methacrylate)
  Sample density R0 = 1.186 g/cc, bulk sound velocity C0 = 2.65 km/s, longitudial sound velocity Cl = 2.72 km/s
  Sample thickness 8.28 mm 
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 1900 +/- 70 m/s
Experiment type: Laser interferometer (VISAR) 

     t, mks     V, m/s

      0.000      0.000
      0.030    298.000
      0.030   2202.000
      0.035   2400.000
      0.040   2430.000
      0.050   2434.000
      0.060   2436.000
      0.070   2434.000
      0.080   2431.000
      0.090   2427.000
      0.120   2415.000
      0.140   2404.000
      0.190   2378.000
      0.240   2355.000
      0.290   2337.000
      0.340   2323.000
      0.390   2311.000
      0.410   2307.000
      0.420   2306.000
      0.440   2307.000
      0.460   2309.000
      0.470   2308.000
      0.490   2305.000
      0.540   2295.000
      0.590   2285.000
      0.640   2277.000
      0.690   2269.000
      0.740   2262.000
      0.790   2255.000
      0.840   2250.000
      0.890   2245.000
      0.940   2239.000
      0.990   2234.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)