Quartz, R0 =  2.650 g/cc

Target: Quartz single crystal (X-cut)
  Sample density R0 = 2.65 g/cc, bulk sound velocity C0 = 3.69 km/s, longitudial sound velocity Cl = 5.57 km/s
  Sample thickness 1.98 mm 
  Aluminum baseplate 2.9 mm thick
Loading: 
  Aluminum impactor 0.2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.006    300.000
      0.008    340.000
      0.010    348.000
      0.019    358.000
      0.034    360.917
      0.046    356.000
      0.058    335.000
      0.066    316.000
      0.082    274.568
      0.100    235.000
      0.117    196.402
      0.137    154.000
      0.157    114.000
      0.183     73.000
      0.190     75.000
      0.208     57.000
      0.268     21.000
      0.276     38.000
      0.289     28.000
      0.314     38.660
      0.350     55.000
      0.372     65.000
      0.400     60.000
      0.430     50.000
      0.460     44.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)