Copper, R0 =  8.930 g/cc

Target: Copper single crystal
  Sample density R0 = 8.93 g/cc, bulk sound velocity C0 = 3.96 km/s, longitudial sound velocity Cl = 4.6 km/s
  Sample thickness 4.35 mm 
Loading: 
  Aluminum impactor 0.2 mm thick, impactor velocity 660 +/- 20 m/s
  (in direction <111>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.100      2.000
      0.150      5.000
      0.200      9.000
      0.205     11.000
      0.210     15.000
      0.215     28.000
      0.230    150.000
      0.235    162.000
      0.241    163.000
      0.245    162.000
      0.250    160.000
      0.259    155.979
      0.265    150.688
      0.308     85.000
      0.320     67.795
      0.340     44.444
      0.349     36.261
      0.360     30.000
      0.370     27.000
      0.383     26.500
      0.385     27.000
      0.400     29.000
      0.450     36.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)