Sapphire, R0 =  3.977 g/cc

Target: Al2O3 (ruby)
  Sample density R0 = 3.99 g/cc, longitudial sound velocity Cl = 11.2 km/s
  Sample thickness 2.21 mm 
  Aluminum baseplate 4.37 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 1250 +/- 50 m/s
  (perpendicular to {1120})
Experiment type: Laser interferometer (VISAR) (water window)

     t, mks     V, m/s

      0.000      0.000
      0.020      5.000
      0.032     10.000
      0.040     20.000
      0.040     55.770
      0.050    513.270
      0.050    555.000
      0.080    513.270
      0.132    417.143
      0.160    360.770
      0.200    266.090
      0.222    210.370
      0.265    115.979
      0.290     61.070
      0.294    117.672
      0.300    266.090
      0.310    383.030
      0.315    410.000
      0.322    416.500
      0.330    418.590
      0.340    410.000
      0.370    360.770
      0.420    266.090
      0.450    208.270
      0.490    113.590

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)