Steel 35h3NM, R0 =  7.760 g/cc

Target: 
  Sample density R0 = 7.76 g/cc, bulk sound velocity C0 = 4.65 km/s, longitudial sound velocity Cl = 5.89 km/s
  Sample thickness 15 mm (rod, batch I)
Loading: 
  High explosive in contact with sample
  (in the lateral direction)
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.070     90.000
      0.350    137.000
      0.500    443.000
      0.590    450.000
      0.997    446.914
      1.590    434.000
      2.090    409.000
      2.590    384.000
      3.090    352.000
      3.590    323.000
      4.120    295.000
      4.460    282.000
      4.550    293.000
      4.650    307.000
      4.840    334.000
      4.970    354.000
      5.350    386.000
      5.480    390.000
      5.570    390.000
      5.690    386.000
      6.090    360.000
      6.320    345.000
      6.590    331.000
      6.850    321.000
      7.090    318.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)