Aluminum AD1, R0 =  2.710 g/cc

Target: 
  Sample density R0 = 2.71 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 9.28 mm (rod, batch II)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.170      1.740
      0.213      9.350
      0.348     27.510
      0.427    605.573
      0.481    619.380
      0.556    614.885
      0.624    600.400
      0.674    577.400
      0.710    560.988
      0.749    537.848
      0.814    519.900
      0.863    500.317
      0.920    479.650
      0.964    459.850
      0.995    479.650
      1.039    496.900
      1.107    521.481
      1.197    528.254
      1.313    519.900
      1.415    496.900
      1.522    466.780
      1.597    496.900
      1.680    519.900
      1.748    525.800
      1.840    519.900
      1.952    496.900
      2.048    468.910
      2.145    496.900
      2.230    519.900
      2.306    524.740
      2.390    519.900
      2.510    496.900
      2.596    467.670
      2.682    496.900
      2.775    516.684
      2.860    521.000
      2.943    516.684
      3.025    496.900
      3.111    466.090
      3.197    496.900
      3.307    519.900
      3.404    516.684
      3.533    495.802

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)