Aluminum AD1, R0 =  2.710 g/cc

Target: 
  Sample density R0 = 2.71 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10 mm (rod, batch II)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.032      2.780
      0.086      3.080
      0.097     13.070
      0.173     18.600
      0.237     40.250
      0.270     80.500
      0.281    523.250
      0.284    577.720
      0.316    617.970
      0.355    635.000
      0.409    635.767
      0.475    617.970
      0.507    603.750
      0.561    577.720
      0.605    563.500
      0.699    537.470
      0.745    523.250
      0.805    497.220
      0.859    472.800
      0.879    495.802
      0.917    523.250
      0.970    535.309
      1.036    539.720
      1.123    537.848
      1.216    521.481
      1.316    497.220
      1.380    485.070
      1.410    497.220
      1.481    518.942
      1.552    528.254
      1.652    523.250
      1.827    497.220
      1.891    494.440
      1.976    497.220
      2.116    512.260
      2.397    497.180
      2.677    510.070
      2.872    494.790

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)