Aluminum AD1, R0 =  2.710 g/cc

Target: 
  Sample density R0 = 2.71 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10.3 mm (rod, batch II)
  Initial temperature 220 C
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.108      1.110
      0.151     10.150
      0.257     24.720
      0.283     64.970
      0.302    132.300
      0.315    588.220
      0.334    655.550
      0.361    690.710
      0.396    694.744
      0.438    690.229
      0.505    668.720
      0.549    655.550
      0.616    634.074
      0.700    615.300
      0.777    589.771
      0.819    575.050
      0.862    563.960
      0.895    577.919
      0.938    594.286
      0.991    600.420
      1.247    588.220
      1.358    577.460
      1.530    593.360
      1.750    587.231
      1.940    580.850
      2.069    586.720
      2.414    581.010

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)