Aluminum AD1, R0 =  2.710 g/cc

Target: 
  Sample density R0 = 2.71 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10.1 mm (rod, batch II)
  Initial temperature 410 C
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.108      0.690
      0.194     18.960
      0.261     44.950
      0.325    622.504
      0.355    636.332
      0.432    638.970
      0.461    631.817
      0.503    622.504
      0.558    608.450
      0.608    592.028
      0.675    568.200
      0.756    542.210
      0.821    518.430
      0.881    540.670
      0.933    549.982
      1.004    556.410
      1.112    552.240
      1.231    542.210
      1.339    523.260
      1.490    542.210
      1.566    544.370
      1.706    542.210
      1.868    541.300
      2.117    547.220
      2.372    541.090
      2.549    542.210
      2.647    547.270
      2.808    542.210
      2.987    539.700

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)