Aluminum AD1, R0 =  2.710 g/cc

Target: 
  Sample density R0 = 2.71 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10 mm (rod, batch II)
  Initial temperature 525 C
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.216      1.590
      0.238     13.690
      0.297     28.960
      0.336     53.940
      0.360    552.210
      0.379    577.190
      0.392    592.460
      0.433    617.440
      0.498    632.710
      0.540    636.332
      0.599    631.817
      0.649    617.440
      0.716    592.460
      0.758    577.190
      0.826    552.210
      0.888    520.280
      0.922    552.210
      0.974    577.190
      1.000    582.110
      1.061    585.610
      1.158    577.190
      1.353    559.860
      1.570    574.670
      1.916    558.390
      2.057    572.050
      2.425    565.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)