Aluminum AD1, R0 =  2.710 g/cc

Target: 
  Sample density R0 = 2.71 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10.2 mm (rod, batch II)
  Initial temperature 565 C
Loading: 
  Aluminum impactor 1.93 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.236      1.890
      0.301      0.000
      0.333      1.990
      0.372     31.540
      0.408     56.550
      0.456    635.290
      0.483    660.300
      0.537    660.570
      0.602    652.698
      0.685    635.290
      0.741    620.050
      0.830    595.040
      0.891    579.800
      0.966    551.710
      1.020    579.800
      1.083    592.028
      1.131    596.920
      1.183    595.040
      1.331    579.800
      1.438    568.300
      1.524    579.800
      1.653    588.790
      1.846    579.800
      1.954    573.650
      2.040    579.800
      2.121    587.240
      2.340    579.800
      2.395    577.870
      2.627    588.600
      2.901    582.020

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)