Aluminum AD1, R0 =  2.710 g/cc

Target: 
  Sample density R0 = 2.71 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10.23 mm (rod, batch II)
  Initial temperature 610 C
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.237      1.350
      0.259     19.400
      0.281     48.440
      0.324     40.830
      0.338     88.680
      0.350    140.600
      0.369    573.480
      0.374    592.028
      0.384    613.880
      0.400    629.277
      0.453    639.940
      0.529    641.030
      0.637    625.400
      0.678    613.880
      0.766    585.000
      0.806    573.480
      0.870    552.430
      0.897    573.404
      0.950    590.000
      1.025    600.010
      1.144    590.000
      1.295    577.810
      1.423    590.720
      1.770    572.230
      2.050    569.830
      2.590    571.960

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)