Aluminum AD1, R0 =  2.710 g/cc

Target: 
  Sample density R0 = 2.71 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10.17 mm (rod, batch II)
  Initial temperature 645 C
Loading: 
  Aluminum impactor 1.95 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.150      0.990
      0.173     20.710
      0.182     45.670
      0.251     71.190
      0.256    141.910
      0.281    555.990
      0.302    629.277
      0.351    669.065
      0.400    680.635
      0.460    683.810
      0.514    678.377
      0.556    667.110
      0.608    650.230
      0.661    654.956
      0.758    647.560
      0.823    647.740
      0.962    641.930
      1.036    645.860
      1.122    642.780
      1.389    637.260
      1.816    634.420
      2.244    623.310

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)