Aluminum AMg6M, R0 =  2.610 g/cc

Target: 
  Sample density R0 = 2.61 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 4.4 mm (sheet)
Loading: 
  Aluminum impactor 0.2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.020     42.000
      0.060     58.000
      0.090     76.000
      0.095     87.000
      0.100    110.000
      0.112    256.720
      0.120    279.000
      0.140    263.000
      0.180    195.000
      0.195    162.000
      0.220    123.000
      0.230    115.000
      0.280    135.000
      0.310    115.000
      0.330    102.000
      0.366    119.259
      0.380    122.000
      0.450     95.000
      0.490    107.000
      0.520    104.000
      0.560     95.000
      0.590    103.000
      0.620     99.000
      0.670    101.000
      0.780    100.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)