Aluminum AMg6M, R0 =  2.610 g/cc

Target: 
  Sample density R0 = 2.61 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 7 mm (sheet)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 1900 +/- 70 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.020      3.000
      0.040      9.000
      0.065     20.000
      0.075    150.000
      0.075    199.000
      0.075   1705.000
      0.075   1750.000
      0.090   1840.129
      0.120   1857.000
      0.169   1862.000
      0.260   1857.000
      0.341   1840.129
      0.399   1815.147
      0.509   1734.000
      0.585   1793.000
      0.625   1808.000
      0.669   1813.000
      0.708   1806.143
      0.879   1736.000
      1.041   1779.541
      1.089   1786.000
      1.129   1779.541
      1.279   1741.000
      1.380   1766.000
      1.449   1773.000
      1.510   1766.000
      1.639   1743.000
      1.765   1764.000
      1.819   1769.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)