Aluminum AMg6M, R0 =  2.610 g/cc

Target: 
  Sample density R0 = 2.61 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10 mm (sheet)
  Copper baseplate 4 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 3000 +/- 100 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.070      0.000
      0.077      4.000
      0.083     20.000
      0.085    150.000
      0.085    199.000
      0.095   2605.000
      0.095   2670.000
      0.098   2760.000
      0.098   2780.000
      0.104   2783.000
      0.110   2780.000
      0.269   2643.000
      0.313   2658.857
      0.334   2662.000
      0.374   2658.000
      0.450   2645.000
      0.480   2655.000
      0.509   2660.000
      0.535   2656.429
      0.614   2637.000
      0.655   2647.000
      0.691   2651.000
      0.725   2647.000
      0.789   2635.000
      0.840   2642.000
      0.864   2644.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)