Magnesium Mg95, R0 =  1.738 g/cc

Target: Magnesium Mg95, "original" cast magnesium
  Sample density R0 = 1.738 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 10.09 mm (bar)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.216      4.890
      0.248     61.390
      0.257    107.360
      0.310    677.860
      0.345    815.060
      0.363    846.914
      0.410    858.630
      0.459    855.732
      0.533    840.860
      0.607    808.818
      0.695    762.258
      0.765    715.697
      0.808    680.423
      0.863    654.880
      0.893    677.860
      0.950    713.390
      1.011    738.977
      1.101    745.050
      1.181    738.110
      1.295    713.390
      1.359    725.050
      1.752    734.720
      2.006    726.690
      2.282    730.890
      2.590    731.590

References:
1. G. I. Kanel\', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)