Magnesium Mg95, R0 =  1.738 g/cc

Target: Magnesium Mg95, "original" cast magnesium
  Sample density R0 = 1.738 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 9.95 mm (bar)
  Initial temperature 280 C
Loading: 
  Aluminum impactor 2.01 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.032      4.610
      0.119     20.570
      0.129     52.220
      0.171     92.470
      0.207    181.570
      0.216    253.470
      0.280    774.956
      0.300    825.570
      0.335    865.820
      0.368    877.249
      0.412    877.249
      0.475    865.820
      0.521    853.968
      0.564    836.332
      0.601    815.873
      0.638    795.414
      0.659    776.720
      0.712    736.470
      0.689    751.675
      0.740    710.758
      0.754    696.220
      0.799    664.570
      0.832    642.320
      0.839    696.220
      0.856    746.032
      0.878    772.134
      0.914    792.593
      0.961    798.960
      1.017    792.593
      1.104    769.312
      1.199    745.070
      1.338    725.573
      1.571    748.854
      1.889    759.080
      2.140    757.672

References:
1. G. I. Kanel\', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)