Magnesium Mg95, R0 =  1.738 g/cc

Target: Magnesium Mg95, "original" cast magnesium
  Sample density R0 = 1.738 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 10.09 mm (bar)
  Initial temperature 320 C
Loading: 
  Aluminum impactor 1.94 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.278      7.070
      0.280    100.250
      0.310    833.750
      0.316    883.980
      0.337    912.169
      0.375    927.610
      0.450    923.810
      0.537    905.200
      0.599    882.892
      0.720    833.750
      0.792    795.414
      0.861    754.497
      0.905    722.399
      0.957    685.640
      0.984    722.399
      1.019    763.316
      1.079    802.480
      1.161    833.750
      1.237    838.740
      1.302    833.750
      1.394    802.480
      1.560    737.530
      1.728    801.411
      1.830    812.800
      1.911    804.233
      2.110    759.690
      2.411    787.380
      2.713    770.180

References:
1. G. I. Kanel\', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)