Magnesium Mg95, R0 =  1.738 g/cc

Target: Magnesium Mg95, "original" cast magnesium
  Sample density R0 = 1.738 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 9.84 mm (bar)
  Initial temperature 495 C
Loading: 
  Aluminum impactor 2.03 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.000      1.660
      0.067      2.510
      0.108     22.280
      0.135     44.590
      0.154     62.680
      0.188     84.990
      0.202    103.080
      0.262    125.390
      0.348    771.790
      0.363    795.414
      0.390    812.190
      0.412    818.111
      0.422    822.290
      0.459    821.869
      0.528    812.190
      0.590    795.414
      0.656    771.790
      0.706    749.480
      0.739    731.390
      0.776    709.080
      0.799    690.990
      0.835    669.841
      0.861    649.735
      0.887    628.280
      0.907    612.620
      0.923    629.277
      0.943    650.590
      0.966    669.841
      0.993    687.478
      1.036    710.758
      1.097    725.573
      1.158    731.760
      1.212    722.399
      1.278    709.080
      1.354    690.990
      1.443    671.620
      1.571    690.990
      1.725    694.880
      1.965    680.640
      2.205    683.470
      2.859    680.520

References:
1. G. I. Kanel\', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)