Magnesium Mg95, R0 =  1.738 g/cc

Target: Magnesium Mg95, "original" cast magnesium
  Sample density R0 = 1.738 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 9.96 mm (bar)
  Initial temperature 555 C
Loading: 
  Aluminum impactor 2.01 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.139      1.690
      0.150     41.350
      0.246     64.180
      0.290    104.930
      0.310    128.160
      0.340    186.430
      0.360    267.930
      0.379    349.430
      0.426    821.869
      0.449    861.660
      0.484    882.892
      0.534    887.790
      0.601    882.892
      0.673    861.660
      0.725    836.332
      0.812    780.160
      0.837    756.930
      0.887    725.490
      0.900    751.675
      0.922    792.593
      0.959    824.691
      1.003    830.688
      1.068    824.691
      1.325    805.470
      1.538    810.020
      1.816    805.500
      2.350    803.840

References:
1. G. I. Kanel\', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)